TRAVELERS between Harrisburg and Altoona, Pennsylvania, can hardly help noticing a ragged, serrated line of mountains stretching off toward the northeast, not far from a busy mountain town called Tyrone. This particular range is conspicuous not on account of its height, but because the rock strata of which it is composed are literally turned on their edges, giving it the abrupt, serrated appearance of some titanic saw. As one approaches nearer, he notices its peculiar, scarred appearance, and a closer view reveals the cause in large numbers of men engaged in blasting and quarrying at its rocky sides. From the main line of the railroad run off numerous branches and side-tracks, terminating at long, low buildings scattered along the bases of the mountains for several miles.
Those rough and ragged mountains are the foundation on which has been built a great and important American industry, the manufacture of plate glass. They are composed of silica, unmixed with mica and other impurities that render ordinary sandstones worthless for this purpose. From them hundreds of thousands of tons of rock are blasted, to be ground into white sand in the crushers in the valley, and then shipped to scores of plate-glass manufacturing establishments located all through Pennsylvania and adjoining States. Within ten days after the quarrymen have blasted the rock from the mountainside, it may be transformed into a show-window for a great department store, or may be fitted into a private residence, ready to be backed with lace curtains.
After the sand arrives at the glass factory, the first step taken consists in mixing the “batch.” This consists of sand, limestone, old glass, soda ash, and various other chemicals. The nature of these chemicals, and the proportion of each of the ingredients, are trade secrets which the manufacturers guard with great care.
The “batch” is placed in a great hopper, and passed through rolls that grind it into a fine powder. Then it is conveyed to the melting pots, composed of fire clay heated to a white heat, inclosed in the furnaces. In these pots the batch boils and bubbles at a temperature of more than twenty-five hundred degrees for twelve hours. By this time it has been changed by the alchemy of heat into glass—a yellow, fiery mass having much the consistency and appearance of Hallow-e'en taffy. The door of the furnace is opened, revealing the melting pot heated to a dazzling white heat by a seething gas fire. The pot is lifted from the furnace, and placed upon a small wagon mounted on casters. The furnace door is closed again, and the workmen rush the wagon to the casting room.
The operation of casting is the crucial point in the manufacture of plate glass. The doors of the casting room are closed, to prevent drafts, and the smallest particle of dust might cause a defect that would ruin the entire cast. At the same time quick action is necessary, as the molten glass cools very rapidly, and must be poured out while still perfectly fluid.
A hydraulic crane with immense iron clamps is lowered over the pot, and this lifts it seven feet above the floor. Several men run up and wipe from the pot every trace of dust and soot. Then the crane carries it over the exact center of the casting table, where its edge is tilted up, allowing the contents to flow quickly out. The casting apparatus consists simply of a steel bed twenty feet square, provided with a heavy steel roller. The moment the molten glass flows upon the table the roller starts on its course, and rolls out a great plate about half an inch in thickness. Almost instantly the plate cools sufficiently to be recognized as glass, translucent and corrugated on both surfaces. If allowed to cool now, the plate would begin to crack in a very few minutes. Two minutes after the pot has been emptied, the rough sheet of glass, still resting upon the casting table, is pushed into the tempering furnace, or lehr.
For the next three and one-half hours no one sees the glass. On a moving bed, like the straw carrier of a threshing-machine, the sheet is carried slowly through a gradually diminishing degree of heat for a distance of one hundred feet. At the farther end of the tempering furnace the sheet is taken out and placed on a wooden rack and allowed to cool.
Next comes the grinding. In order to save time, several sheets are ground at the same time. Mounted on trucks are round, revolving tables, each twenty-four feet in diameter. The sheets are buried on top of these in a thick layer of plaster, and tightly wedged in place. When the plaster sets, the tables are run on the trucks to the middle of the grinding room, and are there placed on another truck that conveys them underneath two “spiders,” fitted with twenty heavy steel grinding “shoes.” The table is connected up with power by means of belts, and revolves at the rate of twenty-four revolutions a minute. The grinding spiders, weighing several tons, revolve in the opposite direction, and water and fine, hard sand begin grinding away the plaster and the corrugated surface of the glass. For three hours the tables are operated with sand, and then for another hour with emery powder. By this time the corrugations have been ground down, so that the upper surface of the sheet of glass is perfectly flat.
The glass plate is then given another coat of plaster, and is ready for the polishing machine. This is operated in exactly the same manner as the grinding machine, except that the spiders are fitted with shoes covered with felt. After three hours under the polishers, a fine, transparent surface is put on the glass. The sheet is then turned, and the other side is subjected to the same processes. Then the sheets are placed in a rack, and washed with water and a mild solution of sulphuric acid. Then they are taken to the cutting room, and given a final polishing off, to be ready for the inspector.
What would pass for a perfect sheet of crystal under the eye of an untrained observer often fails to meet the requirements of the inspector. He makes a critical examination of every square inch of the surface before pronouncing it perfect. Sometimes he merely runs his hand over the glass, and then orders it back to the polishing room for more perfect finishing. Air bubbles, scratches, and blemishes of various kinds are detected and marked with a piece of chalk. If these are of such a nature that they can not be removed by further polishing, the sheet must be cut into sizes that will allow of cutting out the imperfections entirely. Then comes the cutter. With his diamond and rule, he soon converts the irregular sheet into “lights” of standard measurements.

The glass is then finished. The time required to carry it from the casting tables to the cutters is less than twenty-four hours. From the mixing of the raw sand in the batch to the final boxing and stenciling of the finished product requires about forty-eight hours. Frequently the finished plates of glass are shipped from the factory in the same car that conveyed thither the identical sand out of which those plates were made. The rocks blasted from the mountainside are often transformed into window lights and put in position in a building in less than two weeks’ time.
However, it is in mirrors that the highest manufactured form of the mountain sandstone is seen. The plates of glass are first cut into the required sizes, and then beveled on rapidly revolving emery wheels. When the beveled edge has been cut down far enough, it is polished by wheels of felt. For both beveling and polishing the plate of glass is held lightly against the wheel by the workmen. As soon as both surfaces of the glass, including the beveled edges, have been reduced to a condition of as nearly perfect smoothness as is possible, the plate is passed on to the silvering department.
An amalgam of mercury and tin was formerly used for backing mirrors; but mirrors made in this way reflect but imperfectly, and the workmen are exposed to the certainty of sooner or later contracting mercurial poison. For this reason nitrate of silver is now used exclusively for this purpose. This is dissolved in ammonia, and then precipitated by a solution of tartaric acid. The plates of glass are then placed, face down, on warm metallic tables, and the solution poured over them. The heat causes the silver to be precipitated and to adhere to the glass. As soon as this hardens, it is given a coat of shellac, and then one of paint. The plates are then ready for their frames, and the rough, unsightly sandstone has been transformed into a beautiful and useful mirror for the adornment of our homes.—John L. Cowan, in The Children’s Visitor.